An ultrasonic cleaner removes rust when the bath holds a chemistry that dissolves or lifts the oxide. The ultrasonics keeps fresh solution at the surface and carries it into holes, threads and pits. On steel and cast iron, use MetalTek 100: one caustic bath takes the grease, the rust and old paint off. Keep aluminium, zinc and brass out of it. Then rinse and protect the bare steel, because it can start to rust again within the hour.
Why water alone does not take rust off
Rust is iron oxide grown out of the metal itself. It is not dirt sitting on top. A degreaser in a heated tank takes the oil and loose soil off and leaves the oxide behind.
To remove rust, the chemistry has to convert the oxide to something soluble, or lift it off the base metal. The ultrasonics does the work of a brush in places a brush cannot reach: inside bores, under heads of bolts, down threads and in pitting.
Acid or caustic: two different routes to the same bare steel
Our page on contaminant science puts rust and scale on the acid side, and that is right about dissolving them. An acid turns the oxide into a soluble salt and carries it away in the bath.
A caustic alkaline works the other way. It does not dissolve the oxide. It attacks the grease and the paint film holding everything on, and the oxide lifts off with them. That is why one caustic bath can take grease, rust and old paint together, and why it is not a contradiction that a pH 14 product removes rust.
Which route you want depends on the part. The acid route is faster on heavy mill scale and heat tint, and it needs a tank built for acid. The caustic route does three jobs in one bath and runs in a stainless tank. Neither one puts metal back where the rust has eaten in.
The rust remover for steel and cast iron
| Chemistry | How it works | Dose and heat | Use it on | Keep out |
|---|---|---|---|---|
| MetalTek 100 | Caustic alkaline, pH 14. Takes grease, rust and old paint off in one bath | 10–30% · 60–80 °C, never above 80 °C | Iron and steel only | Aluminium, zinc, tin, brass, bronze, plated finishes, glass |
Figures are from each product’s data sheet. The data sheet governs, and a trial on your parts sets the exact time. Prices and the rest of the range are on ultrasonic cleaning solution. Not sure which one? Use the chemical selector.
Which one for which job
Rusty steel with oil and old paint on it
MetalTek 100. It degreases, derusts and strips paint on iron and steel in one bath, so the part does not go through three tanks. Sort the load first: any aluminium, zinc or brass in the basket will be attacked.
Heat scale and heat tint on stainless
This is descaling, not rust removal: use Descale. Run it in a polypropylene insert tank, never left standing in a stainless ultrasonic tank, and extract the acid mist. Bake hardened or high-tensile steel within 4 hours of pickling.
How to do it, step by step
- Check the metal. Find out what every part in the load is made of before you pick the chemistry. The metal decides first, the rust second.
- Degrease heavy oil first. Oil stops the chemistry reaching the rust. On steel and cast iron MetalTek 100 does both at once: the one caustic bath takes the grease and the rust.
- Make up the bath. Add the concentrate at the dose for your chemistry and heat the tank to working temperature. The dosage calculator works out the litres.
- Load the basket. Single layer where you can, holes and threads up or sideways, parts off the tank floor. See how to load the basket.
- Run the ultrasonics and check the parts. Use the shortest cycle that takes the rust off. Lift a part out and look, rather than leaving the load in longer than it needs.
- Rinse. Flush the chemistry out of threads and bores. MetalTek 100 rinses off with water: rinse thoroughly before drying.
- Protect the bare steel. Dip in Anti-Rust at 2–5% for one to two minutes and do not rinse it off. Keep Anti-Rust off aluminium, zinc, brass and copper.
- Dry. Hot-air dry so the part leaves the line dry inside and out.
A job with the settings
Cast iron engine blocks and heads, in a heavy-duty alkaline deruster at 15–20%, 70–80 °C, 40 kHz, one to two hours of wash time. Rust in the water jacket, carbon in the galleries and old paint on the faces came off in one immersion. Then a hot rinse and an anti-rust dip. Full write-up: engine block and head cleaning.
Coolers and heat exchangers with scale and oil sludge are cleaned with CoreKleen HX and Descale, with no rodding and no damage to the fins. See radiator and heat exchanger cleaning.
Why your part flash-rusts after cleaning, and how to stop it
A clean part rusts because the tank did its job: the oil and the oxide that were keeping air and water off the steel are gone, and bare iron, warm and wet, rusts within the hour. It is stopped after the tank, in the rinse, the protection and the drying, not by a weaker bath. The full answer, with what makes it worse and the six steps that stop it, is here: Why does my part flash-rust after ultrasonic cleaning, and how do I stop it? Which protection to use, and for how long, is the next question: What corrosion inhibitor or anti-rust should I use after cleaning?
Which machine
The tank needs heat to reach the working temperature of the chemistry. Size it against your largest part, not the litres. See the full range on machines, or ultrasonic parts cleaners for workshop work.
Questions we are asked
Will an ultrasonic cleaner remove rust with just water?
No. Water and a degreaser take oil and loose dirt off, but rust is an oxide grown out of the metal. The bath needs a chemistry that takes it off. On steel and cast iron, that is MetalTek 100.
Can I remove rust from aluminium or zinc parts in the same load?
Not in MetalTek 100. It attacks aluminium and zinc, so sort them out of the basket before the bath.
How long does rust removal take?
Cast iron blocks in a heavy-duty alkaline deruster took one to two hours of wash time at 70 to 80 °C. A trial on your parts sets the exact time.
Why do parts rust again after cleaning?
A freshly cleaned iron or steel part is bare, warm and wet, and rust bloom can start within the hour. Rinse hot, dip in Anti-Rust at 2 to 5% for one to two minutes, leave the film on and dry hot. The section above sets out what makes it worse and the five steps that stop it.
Can I put acid descaler straight into a stainless ultrasonic tank?
No. Run Descale in a polypropylene insert or an acid-resistant tank, and never leave it standing in a stainless ultrasonic tank. Keep it below 60 °C and extract the mist.
Does derusting damage the part?
A caustic bath attacks the base metal as well as the rust if the part stays in too long, so use the shortest cycle that works.
Does Anti-Rust stop flash rust for good?
No. It is in-process protection for hours to days between operations. For storage, or for a part going to paint, use a paintable film or a displacing spray, quoted on request.
Related: How to remove carbon from engine parts · Cleaning mixed metals together · Does ultrasonic cleaning damage aluminium? · How to clean a radiator core
Send us a rusty part
Tell us what the part is made of and what is on it. We clean it and send back the result with the settings used.